金属热处理 ›› 2021, Vol. 46 ›› Issue (11): 178-181.DOI: 10.13251/j.issn.0254-6051.2021.11.030

• 工艺研究 • 上一篇    下一篇

淬火温度对低合金耐蚀27CrMo48VNb钢油井管组织的影响

顾顺杰, 吕传涛, 肖旭, 丁磊, 李阳, 陈鹏飞   

  1. 天津钢管制造有限公司, 天津 300301
  • 收稿日期:2021-06-02 出版日期:2021-11-25 发布日期:2021-12-08
  • 作者简介:顾顺杰(1989—),男,工程师,硕士,主要研究方向为抗腐蚀油井管,E-mail:g897559203@126.com
  • 基金资助:
    国家重点研发计划(2019YFF0217500,2019YFF0217502)

Effect of quenching temperature on microstructure of low alloyed corrosion resistant 27CrMo48VNb steel OCTG

Gu Shunjie, Lü Chuantao, Xiao Xu, Ding Lei, Li Yang, Chen Pengfei   

  1. Tianjin Pipe Corporation, Tianjin 300301, China
  • Received:2021-06-02 Online:2021-11-25 Published:2021-12-08

摘要: 通过系列温度淬火试验对低合金耐蚀27CrMo48VNb钢油井管进行热处理,并采用光学显微镜和透射电镜对不同温度淬火后组织、原奥氏体晶粒以及析出相进行了观察,研究了淬火温度对试验钢组织、晶粒尺寸和析出相的影响。结果表明,试验钢淬火后形成了马氏体组织。随着淬火温度升高,淬火后马氏体组织和原奥氏体晶粒尺寸逐渐增加。当淬火温度为890~1000 ℃时,随着淬火温度升高,晶粒尺寸增加较小;当淬火温度超过1000 ℃时,随着淬火温度升高,原奥氏体晶粒显著粗化。组织和原奥氏体晶粒尺寸随淬火温度的变化趋势与高温析出相溶解析出行为有关。试验钢的淬火温度应控制在890~1000 ℃。

关键词: 低合金耐蚀油井管, 淬火温度, 晶粒尺寸, 析出相

Abstract: A series of quenching treatment at different temperatures were performed on low alloyed corrosion resistant 27CrMo48VNb steel OCTG. The microstructure, prior austenite grain and precipitates of the tested steel quenched at different temperatures were characterized by optical microscope and transmission electron microscope. The effect of quenching temperature on microstructure, grain size and precipitate was analyzed. The results show that the martensite can be observed in the tested steel after quenching. The size of microstructure and prior austenite grain gradually increases with the increase of quenching temperature. When the quenching temperature is 890-1000 ℃, the grain size increases slightly with the increase of quenching temperature; when the quenching temperature exceeds 1000 ℃, as the quenching temperature increases, the prior austenite grains are significantly coarsened. The change trend of microstructure and prior austenite grain size versus quenching temperature is related to the dissolution and precipitation behavior of precipitates at high temperature. Therefore, the quenching temperature from 890 ℃ to 1000 ℃ of the tested steel is recommended.

Key words: low alloyed corrosion resistant OCTG, quenching temperature, grain size, precipitate

中图分类号: