金属热处理 ›› 2021, Vol. 46 ›› Issue (12): 149-155.DOI: 10.13251/j.issn.0254-6051.2021.12.024

• 组织与性能 • 上一篇    下一篇

无钛热冲压成形钢的连续冷却与等温转变规律

耿吴宾1,2, 崔青玲1, 梁佳伟1, 朱宗伟1, 张龙超3   

  1. 1.东北大学 轧制技术及连轧自动化国家重点实验室, 辽宁 沈阳 110819;
    2.育材堂苏州材料科技有限公司, 江苏 苏州 215000;
    3.西昌钢钒有限公司, 四川 西昌 615000
  • 收稿日期:2021-07-22 出版日期:2021-12-25 发布日期:2022-02-18
  • 通讯作者: 崔青玲,副教授,E-mail:cuiql@mail.neu.edu.cn
  • 作者简介:耿吴宾(1995—),男,硕士研究生,主要研究方向为汽车钢,E-mail:gengwubin@qq.com。
  • 基金资助:
    攀西试验区第四批项目——钒纳米析出韧化2 GPa热冲压钢开发

Law of continuous cooling transformation and isothermal transformation of titanium-free hot stamping steel

Geng Wubin1,2, Cui Qingling1, Liang Jiawei 1, Zhu Zongwei1, Zhang Longchao3   

  1. 1. State Key Laboratory of Rolling and Automation, Northeastern University, Shenyang Liaoning 110819, China;
    2. Yucaitang Suzhou Material Technology Co., Ltd., Suzhou Jiangsu 215000, China;
    3. Xichang Steel and Vanadium Co., Ltd., Xichang Sichuan 615000, China
  • Received:2021-07-22 Online:2021-12-25 Published:2022-02-18

摘要: 利用Thermo-Calc热力学软件(TCFE 9数据库)、DIL805A/D变形热膨胀相变仪和场发射扫描电镜(FE-SEM)研究了连续冷却转变及等温转变过程中无钛热冲压成形钢的微观组织演化规律。结果表明:试验钢的Ac1=749 ℃,Ac3=863 ℃。绘制了CCT曲线和TTT曲线;无钛热冲压成形钢的马氏体相变开始温度Ms=385 ℃,马氏体相变结束温度Mf=130 ℃。过冷奥氏体冷却过程中,发生马氏体相变的临界冷却速度为5 ℃/s;当等温温度高于750 ℃时,热冲压成形后可获得全马氏体组织。

关键词: 无钛热冲压成形钢, 连续冷却转变, 等温转变, 临界冷却速度

Abstract: Using Thermo-Calc thermodynamics software (TCFE 9 database), DIL805A/D deformation thermal expansion phase changer and field emission scanning electron microscope (FE-SEM), the law of microstructure evolution of a titanium-free hot stamping steel during continuous cooling transformation and isothermal transformation was studied. The results show that the Ac1 and Ac3 of the steel is 749 ℃ and 863 ℃, respectively, and the corresponding CCT curve and TTT curve are drawn. The martensitic transformation start temperature of the titanium-free hot stamping steel is 385 ℃, and the martensitic transformation finish temperature is 130 ℃. During the cooling process of supercooled austenite, the critical cooling rate for martensite transformation is 5 ℃/s; when the isothermal temperature is higher than 750 ℃, the full martensite structure can be obtained after hot stamping.

Key words: titanium-free hot stamping steel, continuous cooling transformation, isothermal transformation, critical cooling rate

中图分类号: