金属热处理 ›› 2023, Vol. 48 ›› Issue (10): 182-187.DOI: 10.13251/j.issn.0254-6051.2023.10.027

• 工艺研究 • 上一篇    下一篇

时效处理对深冷轧制Al-4.5Cu-1.5Mg-0.1Er合金显微组织与力学性能的影响

谢尚恒1,2, 孙有平1,2,3, 何江美1,2,3, 朱嘉欣1,2, 方德俊1,2   

  1. 1.广西科技大学 机械与汽车工程学院, 广西 柳州 545006;
    2.广西土方机械协同创新中心, 广西 柳州 545006;
    3.广西汽车零部件与整车技术重点实验室, 广西 柳州 545006
  • 收稿日期:2023-03-29 修回日期:2023-07-21 出版日期:2023-10-25 发布日期:2023-12-07
  • 通讯作者: 孙有平,教授,博士,E-mail:syptaiji@126.com
  • 作者简介:谢尚恒(1997—),男,硕士研究生,主要研究方向为金属材料加工,E-mail:894169019@qq.com。
  • 基金资助:
    中央引导地方科技发展专项(桂科ZY21195053);广西重点研发计划(桂科AB23026104);广西高等学校高水平创新团队项目(桂教师范[2019]52号)

Effect of aging treatment on microstructure and mechanical properties of cryorolled Al-4.5Cu-1.5Mg-0.1Er alloy

Xie Shangheng1,2, Sun Youping1,2,3, He Jiangmei1,2,3, Zhu Jiaxin1,2, Fang Dejun1,2   

  1. 1. School of Mechanical and Automotive Engineering, Guangxi University of Science and Technology, Liuzhou Guangxi 545006, China;
    2. Guangxi Earthmoving Machinery Collaborative Innovation Center, Liuzhou Guangxi 545006, China;
    3. Guangxi Key Laboratory of Automobile Components and Vehicle Technology, Liuzhou Guangxi 545006, China
  • Received:2023-03-29 Revised:2023-07-21 Online:2023-10-25 Published:2023-12-07

摘要: 采用光学显微镜(OM)、X射线衍射仪(XRD)、扫描电镜(SEM)和电子万能试验机等研究了时效处理对深冷轧制Al-4.5Cu-1.5Mg-0.1Er合金板材显微组织和力学性能的影响。结果表明,经时效处理后,Al-4.5Cu-1.5Mg-0.1Er合金中析出相数量增多,分布更均匀,主要为S(Al2CuMg)相和θ(Al2Cu)相。随时效温度的升高及时效时间的延长,部分第二相回溶、粗化,造成合金性能下降。深冷轧制态Al-4.5Cu-1.5Mg-0.1Er合金板材经180 ℃×8 h时效处理后获得了最佳综合性能,抗拉强度和断后伸长率分别为541 MPa和11.33%,比深冷轧制态铝合金分别提高了58 MPa和7.11%,此时合金的断裂类型为韧性断裂。

关键词: Al-Cu-Mg-Er合金, 时效处理, 显微组织, 力学性能, 织构

Abstract: Effect of aging treatment on microstructure and mechanical properties of cryorolled Al-4.5Cu-1.5Mg-0.1Er alloy plate was studied by means of optical microscope (OM), X-ray diffractometer (XRD), scanning electron microscope (SEM) and tensile tester. The results show that the amount of precipitated phases in the Al-4.5Cu-1.5Mg-0.1Er alloy after aging is increased and the distribution is more uniform, which are mainly S(Al2CuMg) phase and θ(Al2Cu) phase. As the aging temperature increases and the aging time is extended, part of the second phase redissolves and coarsens, resulting in the degradation of alloy properties. The best comprehensive properties are obtained when the cryorolled Al-4.5Cu-1.5Mg-0.1Er alloy plates are aged at 180 ℃ for 8 h, of which the tensile strength and elongation reach 541 MPa and 11.33%, respectively, improving by 58 MPa and 7.11% compared with that without aging. Meanwhile, the fracture type of the alloy is ductile fracture.

Key words: Al-Cu-Mg-Er alloy, aging treatment, microstructure, mechanical properties, texture