金属热处理 ›› 2021, Vol. 46 ›› Issue (3): 206-212.DOI: 10.13251/j.issn.0254-6051.2021.03.040

• 测试与分析 • 上一篇    下一篇

Cr12MoV钢冲裁模的失效分析与热处理工艺优化

高志玉1, 何维1, 景秀坤2, 樊献金1, 王迎新2, 白江2, 王大亮2   

  1. 1.辽宁工程技术大学 材料科学与工程学院, 辽宁 阜新 123099;
    2.富奥辽宁汽车弹簧有限公司 技术部, 辽宁 辽阳 111005
  • 收稿日期:2020-11-08 出版日期:2021-03-25 发布日期:2021-05-08
  • 作者简介:高志玉(1981—),男,副教授,博士,主要研究方向为金属材料强韧化与材料优化设计,E-mail:zhiyugao@126.com
  • 基金资助:
    辽宁省博士科研启动基金(20170520151);辽宁省教育厅科学研究经费项目(LJ2020JCL021);辽宁工程技术大学创新团队项目(LNTU20TD-16);大学生创新创业训练计划(201810147092,201910147034)

Failure analysis and heat treatment process optimization of Cr12MoV steel blanking die

Gao Zhiyu1, He Wei1, Jing Xiukun2, Fan Xianjin1, Wang Yingxin2, Bai Jiang2, Wang Daliang2   

  1. 1. College of Materials Science and Engineering, Liaoning Technical University, Fuxin Liaoning 123099, China;
    2. Technical Department of Fuao Liaoning Automotive Spring Co., Ltd., Liaoyang Liaoning 111005, China
  • Received:2020-11-08 Online:2021-03-25 Published:2021-05-08

摘要: Cr12MoV钢冲裁模使用时因过度磨损而早期失效,从服役环境、化学成分、硬度、显微组织进行分析,并采用有限元仿真对冲裁模服役时的温度分布进行计算。结果表明:冲裁模化学成分符合标准规定,硬度略低于技术要求,显微组织中共晶碳化物不均匀度及大块碳化物尺寸超出标准规范,现场测试及仿真计算表明冲裁模服役温度较高(<500 ℃)。冲裁模热处理工艺不当,组织存在缺陷,抗回火稳定性及热疲劳性较差,使用过程中因服役温度较高发生回火软化,从而造成冲裁模的早期磨损失效。建议采用具有高淬高回特征的热处理工艺,利用Cr12MoV钢的二次硬化效应赋予冲裁模良好的抗回火稳定性。利用优化后的工艺生产的冲裁模使用寿命提高至原来的4.62倍。

关键词: Cr12MoV钢, 冲裁模, 失效分析, 热处理, 有限元仿真

Abstract: Early failure of Cr12MoV steel blanking die was caused by excessive wear. The service environment, chemical composition, hardness and microstructure were analyzed, and the temperature distribution of the die in service was calculated by finite element simulation. The results show that the chemical composition of the blanking die meets the requirements of the standard, the hardness is slightly lower than the technical requirements, the heterogeneity of eutectic carbides in the microstructure and the size of bulk carbides exceed the standard specification, the field test and the simulation calculation show that the service temperature of the blanking die is higher (<500 ℃). It is found that the causes for the early wear failure of blanking die include improper heat treatment process of the blanking die, defects in microstructure, poor tempering stability and thermal fatigue, tempering softening occuring in the service process due to high temperature. It is suggested that the heat treatment process with the characteristics of high quenching temperature and high tempering temperature should be adopted, and the secondary hardening effect of Cr12MoV steel should be used to give the blanking die good tempering resistance stability. The service life of the blanking die produced by the optimized heat treatment process is 4.62 times of the original one.

Key words: Cr12MoV steel, blanking die, failure analysis, heat treatment, finite element simulation