金属热处理 ›› 2021, Vol. 46 ›› Issue (10): 108-111.DOI: 10.13251/j.issn.0254-6051.2021.10.018

• 工艺研究 • 上一篇    下一篇

退火温度对21Cr-0.3Cu铁素体不锈钢组织性能的影响

尹鸿祥, 张倩, 吴毅, 张恒, 赵飒   

  1. 中国铁道科学研究院集团有限公司 金属及化学研究所, 北京 100081
  • 收稿日期:2021-04-14 出版日期:2021-10-25 发布日期:2021-12-08
  • 通讯作者: 张 倩,主要研究方向为金属材料研究和失效分析工作,E-mail:zhq7942@sina.com
  • 作者简介:尹鸿祥(1986—),男,副研究员,博士,主要研究方向为钢种开发和金属部件实效,E-mail:yhxlloy1314920@yeah.net
  • 基金资助:
    国家重点研发计划(2017YFB0304600)

Effect of annealing temperature on microstructure and properties of 21Cr-0.3Cu ferritic stainless steel

Yin Hongxiang, Zhang Qian, Wu Yi, Zhang Heng, Zhao Sa   

  1. Metal & Chemistry Institute, China Academy of Railway Sciences Co., Ltd., Beijing 100081, China
  • Received:2021-04-14 Online:2021-10-25 Published:2021-12-08

摘要: 通过光学显微镜、拉伸试验及背散射电子衍射,研究了退火温度对21Cr-0.3Cu超纯铁素体不锈钢显微组织、力学性能、成形性能和微观织构的影响。结果表明,试验钢经970 ℃退火时,晶粒细小且均匀,组织处于完全再结晶状态。退火温度低于970 ℃时,再结晶不完全;退火温度高于970 ℃时,再结晶晶粒异常长大,这两种情况均出现混晶组织。试验钢在970 ℃退火时,综合力学性能最佳,抗拉强度为473 MPa,屈服强度为315 MPa,伸长率35.7%。随退火温度的升高,试验钢的平均塑性应变比rm值先增加后减少。当退火温度达到970 ℃时,rm可以达到最大值1.82。γ纤维织构密度变化趋势与rm值一致,退火温度为970 ℃时,γ纤维增强明显,此时其取向密度达到最大值f(g)=20.56,成形性能最佳。

关键词: 铁素体不锈钢, 平均塑性应变比, 退火温度, 织构, 成形性能

Abstract: Effect of annealing temperature on microstructure, mechanical properties, formability, and microtexture of the 21Cr-0.3Cu ultra-pure ferrite stainless steel was studied by means of optical microscope, tensile testing and backscattered electron diffraction. The results show that when the tested steel is annealed at 970 ℃, the grains are fine and uniform, and the structure is in a completely recrystallized state. When the annealing temperature is lower than 970 ℃, the recrystallization is incomplete; while when higher than 970 ℃, the recrystallized grains grow abnormally, and mixed grain microstructure appears in both the cases. When the tested steel is annealed at 970 ℃, the overall mechanical properties are the best, with a tensile strength of 473 MPa, a yield strength of 315 MPa, and an elongation of 35.7%. As the annealing temperature rises, the average plastic strain ratio rm first increases then decreases, getting the maximum value of 1.82 at 800 ℃. The change trend of the γ texture density is consistent with that of the value of average plastic strain ratio rm. When the annealing temperature is 970 ℃, the γ texture is reinforced obviously. At this time, its orientation density reaches the maximum value f(g)=20.56, and the forming performance is the best.

Key words: ferritic stainless steel, average plastic strain ratio, annealing temperature, texture, formability

中图分类号: