金属热处理 ›› 2021, Vol. 46 ›› Issue (7): 18-22.DOI: 10.13251/j.issn.0254-6051.2021.07.004

• 组织与性能 • 上一篇    下一篇

不同两相区淬火温度对9Ni钢组织与性能的影响

李荣斌1,2,3, 秦品强1, 陈永强1, 李珂1, 龙文宇1   

  1. 1.上海理工大学 材料科学与工程学院, 上海 200093;
    2.上海电机学院 材料学院, 上海 201306;
    3.上海电机学院 上海大件热制造工程技术研究中心, 上海 201306
  • 收稿日期:2021-04-02 出版日期:2021-07-25 发布日期:2021-12-10
  • 作者简介:李荣斌(1969—),男,教授,博士,主要研究方向为薄膜材料、材料结构模拟,E-mail:rblesh@126.com。
  • 基金资助:
    上海市大件热制造工程技术中心项目(18DZ253400);临港新片区高新产业和科技创新专项项目(SH-LG-GK-2020-28);上海市地方院校能力建设项目(21010500900)

Effect of different intercritical quenching temperature on microstructure and properties of 9Ni Steel

Li Rongbin1,2,3, Qin Pinqiang1, Chen Yongqiang1, Li Ke1, Long Wenyong1   

  1. 1. Academy of Material Science and Engineering, University of Shanghai for Science and Technology, Shanghai 200093, China;
    2. Academy of Materials, Shanghai Dianji University, Shanghai 201306, China;
    3. Shanghai Engineering Research Center of Large Piece Hot Manufacturing, Shanghai Dianji University, Shanghai 201306, China
  • Received:2021-04-02 Online:2021-07-25 Published:2021-12-10

摘要: 通过SEM、XRD、疲劳试验机、冲击试验机等分析了620~680 ℃区间不同两相区淬火温度对9Ni钢强度和低温冲击性能的影响。结果表明,回转奥氏体含量和稳定性对材料性能影响显著,随着两相区淬火温度的升高,9Ni钢抗拉强度不断增大,而低温冲击性能呈现先升高后降低的非线性趋势。在640 ℃时,试样的回转奥氏体含量最高,达9.65%;断后伸长率最高,达到32.67%;冲击吸收能量最高,常温下达到332.83 J,-196 ℃条件下为297.69 J,总体展现出良好的强韧性。

关键词: 9Ni钢, 两相区淬火温度, 微观组织, 回转奥氏体, 力学性能

Abstract: Effects of different intercritical quenching temperatures in the range of 620-680 ℃ on the strength and low temperature impact property of 9Ni steel were analyzed by means of SEM, XRD, fatigue testing machine, and impact testing machine. The results show that the content and stability of reversed austenite have a significant effect on the material properties. With the increase of intercritical quenching temperature, the tensile strength of the steel continues to increase, while the low temperature impact property presents a nonlinear trend of first increasing and then decreasing. When the intercritical quenching temperature is 640 ℃, the reversed austenite content, the elongation after fracture, the impact absorbed energy of the specimens all are the highest, respectively being 9.65%, 32.67%, 332.83 J at room temperature and 297.69 J at -196 ℃, showing the best match of strength and toughness on the whole.

Key words: 9Ni steel, intercritical quenching temperature, microstructure, reversed austenite, mechanical properties